GJS



All values for separately cast, or side-by-side cast samples.
For cast-on samples, other and different values applies.


MATERIAL GRADE MECHANICAL PROPERTY
Ductile Iron
NS-EN 1563
HB Tensile Strength
Rm (MPa)
Yield Strength
Re (MPa)
Elongation
A5 (%)
EN-GJS-400-18 LT
EN-GJS-HB150

130-175
400
240
18
EN-GJS-400-15
EN-GJS-HB155

135-180
400
250
15
EN-GJS-450-10
EN-GJS-HB185

160-210
450
310
10
EN-GJS-500-7
EN-GJS-HB200

170-230
500
320
7
EN-GJS-600-3
EN-GJS-HB230

190-270
600
370
3
EN-GJS-700-2
EN-GJS-HB265

225-305
700
420
2


MATERIAL GRADE
NS-EN 1563

 HB

Norway
NS 11-

Sweden
SS-14-

Danmark
DS 11303

Germany
DIN 1693

Finland
SFS 2113.-75

England
BS 2789, 1973

USA
ASTM A536

EN-GJS-400-18 LT
EN-GJS-HB150


130-175

SJK 400.3
NS 11338

0717-02 717 GGG 40.3 GRP 370 Grade 370/17 60-40-18

EN-GJS-400-15
EN-GJS-HB155


135-180

SJK 400
NS 11342

0717 716 GGG 40 GRP 400 Grade 420/12 60-40-18

EN-GJS-500-7
EN-GJS-HB200


170-230

SJK 500
NS 11350

0727-02 727 GGG 50 GRP 500 Grade 500/7 65-45-12

EN-GJS-600-3
EN-GJS-HB230


190-270

SJK 600
NS 11360

0732-03 707 GGG 60 GRP 600 Grade 600/3 80-55-06

EN-GJS-700-2
EN-GJS-HB265


225-305

SJK 700
NS 11370

0737-01 708 GGG 70 GRP 700 Grade 700/2 100-70-03